Ipesenti yokwakheka:
Al | Cr | Fe | Mn | C | Si | Ni | Cu | Ti | Okunye | Izinto zomhlaba ezinqabileyo |
4.6-5.8 | 14.5-15.5 | Isiseko | Ubukhulu be-0.7 | ukuya kuthi ga ngo-0.05 | ukuya kuthi ga ngo-0.6 | ukuya kuthi ga ngo-0.6 | … | ukuya kuthi ga ngo-0.6 | Zr≤0.3 | … |
Ucingo lokuchasa:
1)Intsimbi ye-Aluminiyam ye-Iron Chrome
CrAl 14-4, CrAl 15-5, CrAl 20-5, CrAl 25-5, njl.
2)Ucingo lweNichrome
NiCr 80/20, NiCr 70/30, NiCr 60/15, NiCr 35/20
3)Nickel Copper Alloy Wire
I-alloy 30, i-alloy 60, i-alloy 90, i-Constantan Wire
Ukufumana iinkcukacha ezithe vetshe, pls ndwendwela iwebhusayithi yethu okanye usithumelele i-imeyile.
INGCACISO:
1Cr13Al4 | 0.03-12.0 | 1.25±0.08 | 588-735 | >16 | >6 | 950 | >10000 |
0Cr15Al5 | 1.25±0.08 | 588-735 | >16 | >6 | 1000 | >10000 | |
0Cr25Al5 | 1.42±0.07 | 634-784 | >12 | >5 | 1300 | >8000 | |
0Cr23Al5 | 1.35±0.06 | 634-784 | >12 | >5 | 1250 | >8000 | |
0Cr21Al6 | 1.42±0.07 | 634-784 | >12 | >5 | 1300 | >8000 | |
1Cr20Al3 | 1.23±0.06 | 634-784 | >12 | >5 | 1100 | >8000 | |
0Cr21Al6Nb | 1.45±0.07 | 634-784 | >12 | >5 | 1350 | >8000 | |
0Cr27Al7Mo2 | 0.03-12.0 | 1.53±0.07 | 686-784 | >12 | >5 | 1400 | >8000 |
Ukufaneleka:
I-Fecrak i-alloy efanelekileyo kunye nokumelana nokwenyani okugqithisileyo (1.20-1.30 ohm-mm2 / m) edibanisa ukumelana nobushushu ukuya kuthi ga kwi-1450C kwaye kuthiwa iyimfuneko kwiqondo lokushisa eligqithiseleyo. . Inokumelana ne-corrosive ngokugqibeleleyo emoyeni, kwi-argon, kwi-vacuum, i-oxidizing, i-sulphur-equlethe kunye neendawo ze-carboniferous.
I-Cr15Al5 Eurofechral
impahla | ibakala | Igama le-UNS | I-DIN | Ukuxinana | I-ASTM |
fecral | 1.4725 | K 92500 | 17470 | 7.4 | B 603-1 |
Usetyenziso oluphambili:ezikos,izinto ezixhathisayo,iziko lobushushu obuphezulu,izinto zokufudumeza zetubula kushishino kunye nezifudumezi.
Iimpawu zoomatshini T°20°C
Inani lokuqubuda | Ipesenti Yokwandiswa |
>5 amaxesha | >16% |
Iimpawu zePhyscal T°20°C
Ukuqina | Ukuxinana | Ukuqhawula umthwalo | Ubushushu bokusebenza obukhulu 850C | Ukumelana nombane | Imagnethi | Iindawo zokunyibilika (°C) |
200-260 HB | 7.1g/cm3 | 637-784m/pa | 1.30 ohn-mm2/m | Imagnethi | 1400 °C |